2714 Hot Die Steel Chemical composition - (Typical analysis in %)
Standards | DB6 |
| DIN2714 |
| AISI L6 |
| AFNOR | 55NCDVV7 | JIS SKT4 |
55iNiCrMoV | C | Si | Mn | P | S | Cr | Ni | Mo | V |
| 0.50-0.60 | 0.10-0.40 | 0.65-0.95 | <0.015 | <0.004 | 1.00-1.20 | 1.50-1.80 | 0.45-0.55 | 0.07-0.12 |
USA | Europe | Germany | China | Japan | India | R.of Korea | Russia |
AISI/SAE | En | DIN,WNr | GB | JIS | IS | KS | GOST |
A681 L6 | 55NiCrMoV7 | 56NiCrMoV7 | 5CrNiMo | SKT 4 | T55Ni7Cr4Mo5V1 | STF 4 | 4ChMNFS |
Utilized as standard steel for manufacturing passes on of different kinds, press bites the dust, expulsion kicks the bucket, retainer plates, heavily clad trim bites the dust, hot shear sharpened pieces of steels and instrument holder.
Utilized as standard steel for manufacturing passes on of different kinds, press bites the dust, expulsion kicks the bucket, retainer plates, heavily clad trim bites the dust, hot shear sharpened pieces of steels and instrument holder.
PROCESS ROUTE
EAF+LF+VD+UPSET+FORGED+ANNEALED+ROUGH TURNED FOR ROUNDS/MILLED FOR FLATS+OIL QUENCHED AND DOUBLE TEMPERED+ ROUGH TURNED FOR ROUNDS/MILLED FOR FLATS
STEEL PROPERTIES
The special Hot Work Pre-hardened Steel has great toughness and high wear resistance. DB6 Steel is generally supplied in hard, quenched, tempered and also in annealed condition in special cases.Usually it's working hardness is 360-430 BHN. This steel grade is the upgraded version of DIN 2713 for greater efficiency and performance.
APPLICATION
Dies for Specially Drop and Close Die Forgings for Hammers & Mechanical Presses, Die Moulds,Shoe Blocks, Die Holder, Cassettes, Piston Rods, Cranks, Boaster, Shearing Blades, Tools, plastic moulds Etc.
PHYSICAL PROPERTIES
Coefficient of Thermal Expansion at°C | 10 m/(m*K) |
20-100 | 12.1 |
20-200 | 13.1 |
20-300 | 13.2 |
20-400 | 13.5 |
20-500 | 14..1 |
20-600 | 14.3 |
Thermal Conductivity at °C | W/(m/*K) |
20 | 35.0 |
350 | 39.0 |
700 | 36.0 |
HEAT TREATMENT
Soft annealing °C | 650-710 |
Cooling | Furnace |
Hardness HB | max, 240 |
Hardening °C | 840-880 /860-900 |
Quenching | Oil / Air |
Hardness after quenching HRC | 57 / 55 |
Tempering °C after quenching | 100 | 200 | 300 | 400 | 450 | 500 | 550 | 600 | 600 |
in Oil -HRC | 56 | 54 | 52 | 49 | 47 | 46 | 43 | 38 | 34 |